SIRIM QAS International SdnBhd (CompanyNo: 41334-X) CHEMICAL TESTING SECTION, Building 16, No1, Persiaran Data' Menteri, POBox 735, Section 2,4911 Shah Alam, Selangor Daml Ehsan, Malaysia Tel no: 3-55446651/55446658/6662 Fax no: 3-55446688 TEST NO : 26KLO63 PAGE: 1 OF 6 This Test Report refers only to samples snbmitted by the applicant to SIRIM QAS International Sdn Bhd and tested by SIRIM QAS International Sdn Bhd This test report shall not be reproduced, except in full and shall not be used for advertising purposes by any means or forms without written approval from Executive Director, SIRIM QAS International Sdn Bhd Please refer overleaf for Conditions Relating To The Use of Test Report Applicant GROUP STEEL CORP (M) SDN BHD 18 Kawasan Industri Ayer Keroh, Ayer Keroh, 7545 Melaka Prepainted Galvanized Steel Sheet Reference standard/ Method of test 1) ASTMBl17-3: Standard Practice for Operating Salt Spray (Fog) Apparatus 2) ASTM D 61 1: Standard for EValuating Degree of Rusting 11Pail1tedSteel Surfaces 3) ASTM D7142el Standard for Evaluating Degree of Blistering of Paints Description of sample' Received two (2) set samples of Prepainted Galvanized Steel Sheet for testil1g,which Wremarked as; Markin!! 1 Everfresh 3 pieces Sample G (75mm x 15mm) 2 Clean Colorbond 3 pieces Sample B (75mm x 15mm) Date received 24tll April 26 Job No 12658419 Issue date 23rd June 26 ;ioi Senior Technical Executive (HAHNAS MAHBUT) Manager Chemical Testing Section Building 16 SIRIM QAS International Sdn Bhd
NO : 26KLO63 PAGE: 2 OF 6 This report refers only to samples submitted by the applicant to SIRIM QAS International Sdn Bhd and tested by SIRIM QAS International Sdn Bhd This test report shall not be reproduced, except in full and shall not be used for advertising purposes by any means or forms without written approval from Executive Director, SIRIM QAS International Sdn Bhd : Everfresh : 3 pieces Sample G (75mm x 15mm) Test condition: Duration of exposure Temperature exposure zone Salt solution used ph of collected solution Volurne of salt collected in ml/h/8 cm2 : 1 hours : 35 C : 5% of NaCI : 68 : 13 ml/hr No Type of test Results 1 Salt Spray Resistance Test 11 Evaluating degree of rusting on painted steel There was no red rust present The evaluation of white rust was at surface based on ASTM D 61-1 * Rust Grade 9-G (3 % Rusted) 12 Evaluating Degree of Blistering of Paints There were blisters observed at rating size 2 - few based on D714-2e1 Note: * The degree of rusting grade based on ASTM D61-1 is depicted in the Appendix Senior ABD atharon Executive Chemka1 Testing Section SIRIM QAS InternaSonalSdn Bhd
NO : 26KLO63 PAGE: 3 OF 6 This report refers only to samples submitted by the applicant to SIRIM QAS International Sdn Bhd and tested by SIRIM QAS International Sdn Bhd This test report shall not be reproduced, except in full and shall not be used for advertising purposes by any means or forms without written approval from Executive Director, SIRIM QAS International Sdn Bhd : Everfresh : 3 pieces Sample G (75mm x 15mm) Before salt spray exposure '- t 1 hours salt spray exposure AI:JUUL/CliZ HnN - Senior Tt'E1:>!!kal Executive Chemical Testing Section SIR1M QAS tinnai SdoBhd '--
NO : 26KLO63 PAGE: 4 OF 6 This report refers only to samples submitted by the applicant to SIRIM QAS International Sdu Bhd and tested by SIRIM QAS International Sdn Bhd This test report shall not be reproduced, except in full and shall not be used for advertising purposes by any means or forms without written approval from Executive Director, SIRIM QAS International Sdn Bhd : Clean Colorbond : 3 pieces Sample B (75mm x 15mm),- Test condition: Duration of exposure Temperature exposure zone Salt solution used ph of collected solution Volume of salt collected in ml/h/8 cm2 : 1 hours : 35 C : 5% of NaCI : 68 : 13 ml/hr No Type of test Results 1 Salt Spray Resistance Test - 11 Evaluating degree of rusting on painted steel There was no red rust present The evaluation of white rust was at surface based on ASTM D 61-1 * Rust Grade 9-G (3 % Rusted) " T 12 Evaluating Degree of Blistering of Paints There were blisters observed at rating size 6 - few based on D714-2e1 Note: * The degree of rusting grade based on ASTM D61-1 is depicted in the Appendix b <:!" Senior al Executive Chef11ka\ Testing Section sirlm QAS International SdD Bbd
NO : 26KLO63 PAGE: 5 OF 6 This report refers only to samples submitted by the applicant to SIRIM QAS International Sdn Bhd and tested by SIRIM QAS International Sdn Bhd This test report shall not be reproduced, except in full and shall not be used for advertising purposes by any means or forms without written approval from Executive Director, SIRIM QAS International Sdn Bhd : Clean Colorbond : 3 pieces Sample B (75mm x 15mm) Before salt spray exposure t 1 hours salt spray exposure DUL LIZ HARaN Senior Tcal Executive Chemical Testing Section SlRIM QAS mtenwional Sdn Bm
NO : 26KLO63 PAGE: 6 OF 6 This report refers only to samples submitted by the applicant to SIRIM QAS International Sdn Bhd and tested by SIRIM QAS International Sdn Bhd This test report shall not be reproduced, except in full and shall not be nsed for advertising purposes by any means or forms without written approval from Executive Director, SIRIM QAS International Sdn Bhd Appendix : ASTM D 61-1: Standard Painted Steel Surfaces for Evaluating Degree of Rusting on 4t D 61 ; in () '# CI)! ; Q in? '# 1! i I in 8 #- c i (I) " -t C z Q Ii :!! g, :9> () #- UJ! I I ii ' ; ft P fi> "-'" I a '# I I/> '! 1 Q III Z III,, (I) ::t z Q en Qcn>!'g Er! 9 [ I g,!n OQtT1 w t) g'' tc I/> Q ' ;b? - "#- Ii 8: i c> '# :u CI) 8: " z" Qẕ t (I) ::I z Q FIG 1 Examples of Area Percentages